Henan Excellent Machinery Co., Ltd
+86-18337370596

Casting technology of tooth plate parts of mineral sizers

Aug 23, 2022

First ,Tooth plate of mineral sizers, made of ZGMn13, is a group of 6 pieces, wool packed in a circle, rotating crushing raw materials. Although the impact is not large, but because of the requirements of the broken particle size is small and uniform, the design of the use of the surface is nail shaped, strange shape, wear, requires a higher wool assembly accuracy and casting quality.

Second,the main casting process analysis:

1, sand using analysis: from the shape and high precision assembly, it can be seen that the use of ordinary clay sand, because of the difficulty of molding and can not ensure the shape of tooth surface and assembly accuracy, have to use self-hardening sand. My section commonly used self-hardening sand is quartz sand as the main material of CO2 sodium silicate sand, because it is acid sand, chemical sand is easy to produce in high manganese steel casting, need to brush thicker manganese steel paint to solve. We can see that the nail part is not only difficult to brush, but also easy to cause coating accumulation in the tooth tip, so that the finished teeth after pouring are not full. Therefore, we should try to choose and high manganese steel with alkaline sand species, to avoid thick brush coating. Such sand mainly has chromite sand and magnesium violin sand. Chromium sand particle size is fine and uniform, has high forming ability and fire resistance, so that it is easy to get high surface quality, high dimensional precision castings. But its price is expensive, a lot of use will cause the casting production cost is very high. And mineral sizers magnesium olivine sand, because the particle roundness is poor, particle size is uneven, so the forming ability is poor; Its fractiousness is also lower than chromium sand (higher than quartz sand). But because of its relatively cheap price and more widely used in high manganese steel casting. Therefore, this trial production mainly uses magnesium olivine sand as the main material of CO2 sodium silicate sand. The four assembly holes of the mud core using chromium ore as the main material of CO2 sodium silicate sand.

mineral sizers toothed plate

2, parting surface: according to the structure, the parting surface of this piece is only selected in the root arc surface, scheme 1 is the tooth face up, scheme 2 is the tooth face down. The tooth upward is not only difficult to fill, and because of the hard sand is not easy to prick the air hole, resulting in the cavity tooth exhaust difficulty and insufficient pouring. All make the casting teeth full degree is not good. Therefore, the teeth should be selected to face down;

3, riser: according to the structure, this riser on the top surface is difficult to gas cutting grinding, coupled with high manganese steel for paste solidification, the selection of side riser is more appropriate. Therefore, two side risers are placed on the two end faces, which is conducive to filling and gas cutting grinding;

4, wood type: strict requirements of wood type dimensional accuracy. Another note is to make a live piece of the nail, the pin direction must be perpendicular to the parting plane rather than the arc surface, to ensure that it does not hinder the die;

5, coating: the use of magnesium olivine alcohol coating, pay attention to prevent nail tip coating accumulation, here the coating must be thin, difficult to control, also can not brush paint.

Third, the production effect: according to the above method of tooth plate production of mineral sizers, the surface is smooth, the assembly dimension precision is high, the tooth nail is clear and full. After user information feedback, the assembly and use effect are particularly good.

Fourth, Experience:

1. C02 sodium silicate self-hardening sand of magnesium olivine sand is very suitable for casting with high dimensional accuracy, smooth surface and more

The sharp Angle, small groove structure is not easy to brush the coating of high manganese steel small and medium parts;

2. Wool high manganese steel parts of the small deep hole, small deep groove structure using chromite sand CO2 sodium silicate self-hardening sand, can be better

Ensure casting accuracy and prevent sand "burning";

3. the small pointed structure of casting, in self-hardening sand casting, should be as far as possible to adopt downward scheme, to ensure the pointed structure

Shape and fullness.